Geýmek / aşgazana çydamly polat ekwiwalent standartlary
Polat derejesi | SSAB | JFE | DILLIDUR | TyssenkKrupp | Ruukki |
NM360 | - | EH360 | - | - | - |
NM400 | HARDOX400 | EH400 | 400V | XAR400 | Raex400 |
NM450 | HARDOX450 | - | 450V | XAR450 | Raex450 |
NM500 | HARDOX500 | EH500 | 500V | XAR500 | Raex500 |
Geýmek / aşgazana çydamly polat --- Hytaý standarty
● NM360
● NM400
● NM450
● NM500
● NR360
● NR400
● B-HARD360
● B-HARD400
● B-HARD450
● KN-55
● KN-60
● KN-63
NM geýýän çydamly polatdan himiki düzümi (%)
Polat derejesi | C | Si | Mn | P | S | Cr | Mo | B | N | H | Seq |
NM360 / NM400 | ≤0.20 | ≤0.40 | ≤1.50 | ≤0.012 | ≤0.005 | ≤0.35 | ≤0.30 | ≤0.002 | ≤0.005 | ≤0.00025 | ≤0.53 |
NM450 | ≤0.22 | ≤0.60 | ≤1.50 | ≤0.012 | ≤0.005 | ≤0.80 | ≤0.30 | ≤0.002 | ≤0.005 | ≤0.00025 | ≤0.62 |
NM500 | ≤0.30 | ≤0.60 | .001.00 | ≤0.012 | ≤0.002 | .001.00 | ≤0.30 | ≤0.002 | ≤0.005 | ≤0.0002 | ≤0.65 |
NM550 | ≤0.35 | ≤0.40 | ≤1.20 | ≤0.010 | ≤0.002 | .001.00 | ≤0.30 | ≤0.002 | ≤0.0045 | ≤0.0002 | ≤0.72 |
NM geýýän çydamly poladyň mehaniki aýratynlyklary
Polat derejesi | Hasyl güýji / MPa | Dartyş güýji / MPa | Uzalma A50 /% | Gatylyk (Brinell) HBW10 / 3000 | Täsir / J (-20 ℃) |
NM360 | 00900 | 501050 | ≥12 | 320-390 | ≥21 |
NM400 | 50950 | 001200 | ≥12 | 380-430 | ≥21 |
NM450 | 501050 | 501250 | ≥7 | 420-480 | ≥21 |
NM500 | 001100 | ≥1350 | ≥6 | 70470 | ≥17 |
NM550 | - | - | - | ≥530 | - |
Geýmek / aşgazana çydamly polat --- ABŞ standarty
● AR400
● AR450
● AR500
6 AR600
Aşgazan çydamly polat plastinka bar
Baha | Galyňlyk | Ini | Uzynlyk |
AR200 / AR 235 | 3/16 "- 3/4" | 48 "- 120" | 96 "- 480" |
AR400F | 3/16 "- 4" | 48 "- 120" | 96 "- 480" |
AR450F | 3/16 "- 2" | 48 "- 96" | 96 "- 480" |
AR500 | 3/16 "- 2" | 48 "- 96" | 96 "- 480" |
AR600 | 3/16 "- 3/4" | 48 "- 96" | 96 "- 480" |
Aşgazan çydamly polat plastinanyň himiki düzümi
Baha | C | Si | Mn | P | S | Cr | Ni | Mo | B |
AR500 | 0.30 | 0.7 | 1.70 | 0.025 | 0.015 | 1.00 | 0.70 | 0.50 | 0.005 |
AR450 | 0.26 | 0.7 | 1.70 | 0.025 | 0.015 | 1.00 | 0.70 | 0.50 | 0.005 |
AR400 | 0.25 | 0.7 | 1.70 | 0.025 | 0.015 | 1.50 | 0.70 | 0.50 | 0.005 |
AR300 | 0.18 | 0.7 | 1.70 | 0.025 | 0.015 | 1.50 | 0.40 | 0.50 | 0.005 |
Aşgazan çydamly polat plastinanyň mehaniki aýratynlyklary
Baha | Güýç kuwwaty MPa | Dartyş güýji MPa | Uzalma A. | Täsir güýji Charpy V 20J | Gatylyk aralygy |
AR500 | 1250 | 1450 | 8 | -30C | 450-540 |
AR450 | 1200 | 1450 | 8 | -40C | 420-500 |
AR400 | 1000 | 1250 | 10 | -40C | 360-480 |
AR300 | 900 | 1000 | 11 | -40C | - |
Aşgazan çydamly polatdan ýasalan programmalar
23 AR235 plitalary orta könelişme programmalary üçin niýetlenendir, bu ýerde düzümdäki uglerod polatyna garanyňda gowulaşan çydamlylygy hödürleýär.
● AR400 premium aşgazana çydamly polat plitalar bolup, olar ýylylyk bilen işlenýär we gatylaşdyrylýar. Dörediş we nikalaşmak mümkinçilikleri.
4 AR450, AR400-den has az güýç islenýän dürli programmalarda ulanylýan aşgazana çydamly plastinka.
5 AR500 plitalary magdançylyk, tokaý hojalygy we gurluşyk üçin amatly.
6 AR600 umumy aýyrmak, gazyp almak, çelekler we geýim jisimleri öndürmek ýaly ýokary köýnekli ýerlerde ulanylýar.
Aşgazan çydamly (AR) polat plastinka adatça togalanan ýagdaýda ýasalýar. Polat plastinka önümleriniň bu görnüşleri / bahalary agyr şertlerde uzak hyzmat etmek üçin ýörite işlenip düzüldi. AR önümleri dag-magdan / karýer, konweýer, material işlemek we gurluşyk we ýeriň hereketi ýaly ugurlarda dürli goşundylar üçin amatlydyr. Dizaýnerler we zawod operatorlary möhüm komponentleriň hyzmat möhletini uzaltmaga we hyzmatda goýlan her bölümiň agramyny azaltmaga synanyşanlarynda AR plastinka polady saýlaýarlar. Täsir we / ýa-da abraziw material bilen süýşmek bilen baglanyşykly programmalarda könelişen plastinka polatdan peýdalanmagyň peýdalary gaty uludyr.
Abraziw çydamly ergin polat plitalary, adatça süýşmäge we aşgazanyň täsirine gowy garşylyk görkezýär. Garyndynyň düzümindäki ýokary uglerod poladyň gatylygyny we berkligini ýokarlandyrýar, ýokary täsir ýa-da aşgazana garşylygy talap edýän programmalar üçin amatly material bolýar. Carbonokary uglerod polat bilen ýokary gatylygy almak bolýar we polat aralaşmaga gowy garşylyk görkezer. Şeýle-de bolsa, ýylylyk bilen işlenýän garyndy plastinka bilen deňeşdirilende köneliş tizligi ýokary bolar, sebäbi ýokary uglerod polat döwükdir, şonuň üçin bölejikler ýerden has aňsat ýyrtylyp bilner. Netijede, ýokary kömürli polatlar ýokary köýnek üçin ulanylmaýar.